• Mon - Sat : 9:00 - 18:00
  • Sun : day off
  • sale@asynt.net
  • +38 (093) 237 64 50

Sheet steel P265GH / 1.0425

» Products » Flat rolled metal » Structural sheet metal » Sheet steel P265GH / 1.0425

Sheet steel P265GH / 1.0425

The goods can be picked up by self-delivery at metal depots in Kyiv. Also, in agreement with the customer, rolled metal products can be delivered to any region of Ukraine

  • Characteristics
  • Description

P265GH delivery forms

Boiler steel grades

Steel grades
EN 10028

Steel grade DIN

Dimensions mm

Special thicknesses

Thickness

Width

Length up to

P 265 GH

1.0425

3 – 250

1000 – 4000

14,000

7,9,11,13,14,16,18,22,28,32

Chemical Composition of P265GH Steel

EN 10028-2

С

<0,2

Si

<0,4

Mn

0.6-1.4

P

<0,025

S

<0.01

Cr

<0,3

Mo

<0.08

Ni

<0,3

V

<0.02

Nb

<0.02

Ti

<0.03

Al

>0.02

Cu

<0,3

N

<0.012

Fe

Other

Mechanical properties of P265GH material

Didn't find a suitable product?

For more information, please contact us or leave your contact details and we will call you back.



    Per EN 10028-2

    +N

    Nominal thickness, (mm)

    < 16

    16 – 40

    40 – 60

    60 – 100

    100 – 150

    150 – 200

    Minimum yield strength, ReH (MPa)

    265

    255

    245

    215

    200

    185

    Tensile strength (tensile strength) , Rm (MPa)

    410-530

    410-530

    410-530

    410-530

    400-530

    390-530

    Minimum elongation after break, A (%)

    22

    Minimum absorbed energy at 20°C, J (J )

    40

    Minimum absorbed energy at 0°C 32°F], J (J)

    34

    Minimum absorbed energy at -20°C, J (J)

    27

    Yield strength at 50°C, ReH (MPa)

    256

    247

    237

    208

    193

    179

    Yield strength at 100°C, ReH (MPa)

    241

    232

    223

    196

    182

    168

    Yield strength at 150°C, ReH (MPa)

    223

    215

    206

    181

    169

    156

    Yield strength at 200°C, ReH (MPa)

    205

    197

    190

    167

    155

    143

    Yield strength at 250°C, ReH (MPa)

    188

    181

    174

    153

    142

    131

    Yield strength at 300°C, ReH (MPa)

    173

    166

    160

    140

    130

    121

    Yield strength at 350°C, ReH (MPa)

    160

    154

    148

    130

    121

    112

    Yield strength at 400°C, ReH (MPa)

    150

    145

    139

    122

    114

    105